How to Fix Sink Marks in Plastic Injection Molding: Causes and Practical Solutions

Quick answer: A sink mark is a shallow depression on the surface of a plastic part, appearing where the wall is thickest. It happens when the thick section keeps shrinking as it cools, but the gate has already frozen or the packing pressure is too low to feed in more material. The most effective fixes are: first make the wall thickness as uniform as possible (keep ribs and bosses from getting too thick), then run a gate freeze test to confirm the holding time is long enough, and place the gate close to the thick section with a large enough size.

1. What is a sink mark, and where does it usually appear?

As plastic cools from melt to solid inside the mold, its volume shrinks. The surface cools and hardens first while the core is still hot. As the core continues to shrink, it pulls the already-formed surface inward, creating a shallow depression: a sink mark. If the surface is too rigid to be pulled in, the shrinkage stays inside the part and forms a void (also called a vacuum bubble).

Common locations of sink marks:

  • Behind ribs (thin reinforcing walls): a sunken line appears on the cosmetic surface opposite the rib.
  • Behind bosses (cylindrical screw mounts): a round dent appears on the cosmetic surface.
  • Locally thick sections: e.g. solid areas in handles, thick edges and corners.
  • Thick sections far from the gate: packing pressure cannot reach them effectively.

Sink marks are less visible on matte or textured surfaces, but on high-gloss or mirror-finish parts even a few hundredths of a millimeter can be seen.

2. Causes of sink marks

1. Part design

  • Uneven wall thickness: the main root cause. Thicker areas cool more slowly and shrink more.
  • Ribs or bosses that are too thick: where a rib or boss meets the main wall, a locally thick section is formed.
  • Abrupt changes in wall thickness: uneven cooling at thick-to-thin transitions easily causes sink marks or warpage.

2. Mold

  • Gate (the entrance where plastic enters the cavity) too small: the gate freezes before the part, so packing pressure can no longer push material in. Submarine (tunnel) gates are especially prone to this because they are usually small.
  • Gate located too far from thick sections: pressure is lost along the flow path and is insufficient by the time it reaches the thick area.
  • Unbalanced cooling channel layout: any area that runs locally hot is prone to sink marks.

3. Molding conditions

  • Holding time too short: if packing stops before the gate freezes, material can flow back or there is not enough time to feed the part.
  • Insufficient holding pressure.
  • Mold or melt temperature too high: shrinkage increases and cooling time gets longer.
  • Insufficient shot size or too little cushion (the material left in front of the screw at the end of injection): there is no material left to feed during packing.

4. Material

  • Semi-crystalline plastics(such as PP, PE, POM and PA) generally have higher molding shrinkage thanamorphous plastics(such as ABS, PC and PS), so sink marks are more noticeable.
  • High moisture content in the resin or a high ratio of regrind can also make quality less stable.

3. Summary of solutions

ItemTypical recommendation / how to check
Design: rib thicknessA common guideline is about 50–70% of the adjacent wall thickness; use the lower end for cosmetic parts, slightly higher for purely structural parts
Design: bossesBoss wall thickness also follows roughly 50–70% of the nominal wall; the base of the boss can be cored out or separated from the outer wall
Design: uniform wall thicknessAvoid abrupt thickness changes and use gradual transitions; consider coring out thick sections (hollowing solid areas into a uniform wall)
Mold: gate locationPlace it as close to the thick section as possible so the plastic flows from thick to thin
Mold: gate sizeThe gate must be large enough not to freeze before the thick section; if a submarine gate is too small, enlarge it or switch to another gate type
Mold: coolingCheck that cooling channels evenly cover thick areas; add local cooling where needed (extra channels or high-conductivity inserts)
Molding: holding timeUse a gate freeze test to find the freeze time and set holding time above it (usually with a small margin)
Molding: holding pressureIncrease gradually without causing flash or sticking; profiled packing (higher at first, then stepping down) can help
Molding: temperatureModerately lower melt and mold temperatures within the range that still fills properly; adjust mold temperature on the cosmetic side as needed
Molding: cushionMake sure a cushion remains at the end of injection; never let the screw bottom out
Material: selectionFor parts with very high cosmetic requirements, evaluate amorphous or filled grades; confirm drying conditions

How to run a gate freeze test

This is the most direct way to check whether the holding time is long enough:

  1. Keep all other conditions fixed and start with a short holding time (e.g. 1 second).
  2. Increase it by about 0.5–1 second each time, and weigh several stable parts at each setting.
  3. Record holding time versus part weight.
  4. Once the weight stops increasing, that time is the gate freeze time.

If the holding time is shorter than this, parts will be underweight and sink marks are more likely. If the weight keeps increasing even with a very long holding time, the gate is freezing very slowly, and you may need to recheck the gate size and temperatures.

4. Illustrative case

The following is an illustrative case based on common industry scenarios, not measured data from a specific customer.

Scenario: A PP part shows obvious sink marks on the cosmetic surface near a submarine gate. The wall near the gate is about 3 mm thick, the submarine gate is about 1 mm in diameter, holding pressure is set low, and holding time is only 1 second.

Key points of analysis:

  • PP is a semi-crystalline plastic and naturally shrinks more.
  • With a 3 mm wall and a 1 mm gate, the gate is likely to freeze before the part has finished cooling.
  • With only 1 second of holding time, packing probably ends before enough material has been fed in.

Recommended order of improvement:

  1. Run a gate freeze test firstto confirm the actual freeze time, and set the holding time long enough.
  2. Then adjust the holding pressure, or switch to profiled packing.
  3. If adjusting conditions is still not enough, the gate is freezing during packing; at that point, considerenlarging the gate or moving it closer to the thick section.
  4. If cosmetic requirements are high,core outthe thick sections in the part design to make the wall more uniform. This is usually the most fundamental solution.

Adjusting process conditions first, then modifying the mold, and finally changing the design is usually the most time- and cost-efficient order. However, if it is clear from the start that the problem lies in the design (for example, rib thickness close to or greater than the wall thickness), it should be corrected before the mold is made.

5. Frequently asked questions (FAQ)

Q1: Can sink marks be fixed just by adjusting molding conditions?

Minor sink marks can usually be improved by extending holding time and increasing holding pressure. But if the root cause is an overly thick wall or an undersized gate, adjusting conditions often brings side effects such as flash, internal stress or longer cycle times. In that case, the mold or the design needs to be addressed.

Q2: How thick should a rib be to avoid sink marks?

The usual recommendation is 50–70% of the adjacent wall thickness. Stay toward the lower end for cosmetic parts and for high-shrinkage materials such as PP. Ribs that are too thin may not fill completely, so it is best to evaluate this together with your mold maker.

Q3: Why is PP more prone to sink marks than ABS?

PP is a semi-crystalline plastic: its molecules crystallize as it cools, causing greater volume shrinkage. Amorphous plastics such as ABS and PC usually shrink less, so with the same design, sink marks are more visible on PP parts.

Q4: How are sink marks related to voids (bubbles)?

They share the same cause: insufficient feeding of a shrinking thick section. If the surface is pulled inward, you get a sink mark; if the surface has already hardened and cannot move, the shrinkage stays inside as a void. So when fixing sink marks, be careful not to turn them into internal voids.

Q5: Can sink marks be predicted before the mold is made?

Yes. During drawing review, check wall-thickness uniformity, rib and boss proportions and gate location to identify high-risk areas before tooling begins.

If your product has sink mark issues, or you would like a design evaluation before tooling, HENPEN can help assess improvement options.
Contact HENPEN →

Facing an injection molding challenge in product development?

HENPEN offers one-stop service from design drawings and mold making to injection molding.